The first time I've seen someone walk the cup and get silver, usually the travel speed is too slow, but this guy was cranking just making that consistency even more impressive i honestly though they had the camera sped up
this is Super duplex - purge gas flow rate 25+ and note: oxygen level should be 0.005 ppm. Torch gas flow rate 15-20 and must be use gas lens body and cup 10-12. Thank you
Tnx brother god tips Frist watching good explan
The first time I've seen someone walk the cup and get silver, usually the travel speed is too slow, but this guy was cranking just making that consistency even more impressive i honestly though they had the camera sped up
thank you sir
awesome video
im learning argon welding
Caliye jaa
Good job bro
Super slick root 🎉
thank you
Good job
thanks everyone 🥰🥰🥰
Nice video
Thanks
How many amps did you put the root pass?
Root gap 3.2-4mm
Pipe thik 6-11mm
Amp 95-110
🔥
GOOD
Hi from czech
Sir can u show us how to start at bottom section.(please)❤
Will do soon sir 🥰
@@Tigwelding99 thanks❤️
I
I have a few setup questions. What acreage were you welding at? What is your purge gas flow rate? What is your torch gas flow rate?
this is Super duplex - purge gas flow rate 25+ and note: oxygen level should be 0.005 ppm. Torch gas flow rate 15-20 and must be use gas lens body and cup 10-12. Thank you
@@Tigwelding99 can you give any root and hot pass amperage suggestions?
2" to 6" pipe SDSS
Pipe thikness 6 mm to 11 mm
Gas flow follow as i given previous
Amperage 80 to 110
Root gape 3.2 - 4 mm
@Tigwelding99 thank you so much! I currently work on SDSS so I'm always trying to get better.